Component    Wt. %  


C 0.08 - 0.13  
Fe 99.18 - 99.62  
Mn 0.3 - 0.6  
P Max 0.04  
S Max 0.05  


Material Notes: 
Used widely in low strength applications. Good formability, fair machinability, can be hardened by cyaniding. Suitable for magnet core applications

Click here to view available vendors for this material.

Physical Properties Metric English Comments 


Density 7.87 g/cc 0.284 lb/in³  

Mechanical Properties 


Hardness, Brinell 105 105  
Hardness, Knoop 123 123  Converted from Brinell hardness. 
Hardness, Rockwell B 60 60  Converted from Brinell hardness. 
Hardness, Vickers 108 108  Converted from Brinell hardness. 
Tensile Strength, Ultimate 365 MPa 52900 psi  
Tensile Strength, Yield 305 MPa 44200 psi  
Elongation at Break 20 % 20 %  In 50 mm 
Reduction of Area 40 % 40 %  
Modulus of Elasticity 205 GPa 29700 ksi  Typical for steel 
Bulk Modulus 140 GPa 20300 ksi  Typical for steel 
Poisson's Ratio 0.29 0.29  Typical For Steel 
Machinability 55 % 55 %  Based on AISI 1212 steel. as 100% machinability. The machinability of Group I bar, rod, and wire products can be improved by cold drawing. 
Shear Modulus 80 GPa 11600 ksi  Typical for steel 

Electrical Properties 


Electrical Resistivity 1.43e-005 ohm-cm 1.43e-005 ohm-cm  condition unknown 

Thermal Properties 


CTE, linear 20°C 12.2 µm/m-°C 6.78 µin/in-°F  0-100ºC 
CTE, linear 250°C 13.5 µm/m-°C 7.5 µin/in-°F  0-300°C (68-570°F) 
CTE, linear 500°C 14.2 µm/m-°C 7.89 µin/in-°F  0-500°C (68-930°F) 
Specific Heat Capacity 0.448 J/g-°C 0.107 BTU/lb-°F  condition unknown; 50-100°C (122-212°F) 
Specific Heat Capacity at Elevated Temperature 0.498 J/g-°C 0.119 BTU/lb-°F  condition unknown; 150-200°C (302-390°F) 
Specific Heat Capacity at Elevated Temperature 0.519 J/g-°C 0.124 BTU/lb-°F  condition unknown; 200-250°C (390-480°F) 
Specific Heat Capacity at Elevated Temperature 0.536 J/g-°C 0.128 BTU/lb-°F  condition unknown; 250-300°C (480-570°F) 
Specific Heat Capacity at Elevated Temperature 0.565 J/g-°C 0.135 BTU/lb-°F  condition unknown; 300-350°C (570-660°F) 
Specific Heat Capacity at Elevated Temperature 0.59 J/g-°C 0.141 BTU/lb-°F  condition unknown; 350-400°C (660-750°F) 
Specific Heat Capacity at Elevated Temperature 0.649 J/g-°C 0.155 BTU/lb-°F  condition unknown; 400-450°C (750-930°F) 
Specific Heat Capacity at Elevated Temperature 0.729 J/g-°C 0.174 BTU/lb-°F  condition unknown; 550-600°C (1020-1110°F) 
Specific Heat Capacity at Elevated Temperature 0.825 J/g-°C 0.197 BTU/lb-°F  condition unknown; 650-700°C (1200-1290°F) 
Thermal Conductivity 49.8 W/m-K 346 BTU-in/hr-ft²-°F  Typical steel